Lightweight
and robust polybenzoxazine foams were prepared using
a simple sol–gel method based on a commercially available benzoxazine
monomer, BA-a, with hexamethylenediamine as a curing agent and methanol/chloroform
as the solvent. By varying the initial concentrations of organic solutions,
polybenzoxazine foams with densities of 0.2815 g/cm3 (F-20),
0.4798 g/cm3 (F-30), and 0.6731 g/cm3 (F-40)
were prepared. Scanning electron microscopy (SEM) images revealed
that all foams possessed open-cell structures, and the morphology
of the pore walls can be readily tailored by initial concentrations.
As a consequence of the porous structure, the polybenzoxazine foams
showed a low dielectric constant (1.47 at 1 MHz for F-20), low dielectric
loss (0.003 at 1 MHz for F-20), low thermal conductivity (0.0604 W/(m
K) for F-20), and low coefficient of linear expansion value (55.1
ppm/°C for F-20). Moreover, foam F-40 showed a favorable T
g of 191.8 °C, char yield of 46.1%, and
compressive strength of 71.74 MPa. The outstanding comprehensive performances
make the polybenzoxazine foams prepared using this methodology good
candidates as lightweight, robust, and thermally stable matrices for
many functional applications.