The purpose of this in vitro study was to investigate whether different types of experimental and commercial restorative dental materials can protect dentin against acid-induced softening. Experimental composites were prepared with a photocurable mixture of methacrylates and two types of bioactive glass (45S5 and a customized low-Na F-containing formulation). Human dentin samples were prepared from mid-coronal tooth slices and immersed in lactic acid solution (pH = 4.0) at 5 mm from set specimens of restorative material. After 4, 8, 12, 16, 20, 24, 28, and 32 days, surface microhardness of dentin samples and pH of the immersion solution were measured, followed by replenishing of the immersion medium. Microstructural analysis was performed using scanning electron microscopy. The protective effect of restorative materials was determined as dentin microhardness remaining statistically similar to initial values for a certain number of acid additions. Scanning electron microscopy showed a gradual widening of dentinal tubules and proved less discriminatory than microhardness measurements. To produce a protective effect on dentin, 20 wt% of low-Na F-containing bioactive glass was needed, whereas 10 wt% of bioactive glass 45S5 was sufficient to protect dentin against acid-induced demineralization. The anti-demineralizing protective effect of experimental and commercial restoratives on dentin was of shorter duration than measured for enamel in a previous study using the same experimental approach.
This study investigated the potential of adhesive coating for hindering the reactivity of ion-releasing dental restorative materials. Experimental composites were prepared by replacing 10 or 20 wt% of reinforcing fillers with two types of bioactive glass. A glass ionomer, a giomer, and an alkasite were used as representatives of commercial ion-releasing materials. Restorative material specimens were coated with an etch-and-rinse adhesive, 1-step self-etch adhesive, 2-step self-etch adhesive, or left uncoated. The specimens were immersed in a lactic acid solution and ion concentrations were measured in 4 days intervals for 32 days (atomic absorption spectrometry for calcium, UV–Vis spectrometry for phosphate, ion-selective electrode for fluoride, and pH-meter for pH values). The adhesive coating reduced ion release between 0.3 and 307 times, in a significantly material- and adhesive-dependent manner. Fluoride release was most highly impaired, with the reduction of up to 307 times, followed by phosphate and calcium release, which were reduced up to 90 and 45 times, respectively. The effect of different adhesive systems was most pronounced for phosphate release, with the following rankings: uncoated ≥ 2-step self-etch adhesive ≥ 1-step self-etch adhesive ≥ etch-and-rinse adhesive. The differences among adhesives were less pronounced for calcium and fluoride. It was concluded that the resinous adhesive layer can act as a barrier for ion release and diminish the beneficial effects of remineralizing restorative materials.
scite is a Brooklyn-based organization that helps researchers better discover and understand research articles through Smart Citations–citations that display the context of the citation and describe whether the article provides supporting or contrasting evidence. scite is used by students and researchers from around the world and is funded in part by the National Science Foundation and the National Institute on Drug Abuse of the National Institutes of Health.