Although some new-generation CAD/CAM and provisional restoration materials display slight cytotoxicity values, the results are still within the reliable range, and they can safely be used in clinical conditions.
The cytotoxicity of nine soft and hard lining materials (Mollosil Plus, Ufi Gel SC, Visco-gel, Molloplast-B, GC Tissue Conditioner, Vertex Rapid Simplified, GC Reline Hard, Vertex Self-Curing, Ufi Gel hard C) was evaluated using human gingival fibroblasts (HGFs). Twelve disk samples per lining material were prepared and incubated for 24, 48, 72, and 96 h. Cytotoxicity of each lining material's extract on cultured HGFs was measured using XTT assay. Data were analyzed using one-way ANOVA, post hoc Dunnett's T3 and Bonferroni tests at a significance level of p<0.05. At all incubation periods, all the hard lining materials (Vertex-SC, GC Reline Hard, Vertex-RS, and Ufi Gel hard C) showed cell viability higher than 90%. Among the soft lining materials, although there were no significant differences in cell viability among the different incubation periods for each lining material (p>0.05), autopolymerized acrylic-based GC Tissue Conditioner showed significantly lower cell viability than the other soft lining materials at each incubation period. Among the hard lining materials, there were no significant differences both among the materials and across all incubation periods for each lining material (p>0.05). In conclusion, all soft and hard liners exhibited good biocompatibility regardless of incubation time, except for GC Tissue Conditioner.
The aim of this study was to evaluate mechanical properties of six new-generation all-ceramic materials for CAD/CAM (Lava Ultimate [LU], VITA Mark II [VM], InCoris TZI [IC], IPS e.max CAD [EM], VITA Suprinity [VS], IPS Empress CAD [EC]) and two different provisional restoration CAD/CAM materials (Telio CAD [TC], Vita CAD-Temp [VC]) after different storage conditions. 36 bar-shaped samples of 4 mm in width and 14 mm in length with 1.2 mm thicknesses were prepared from each material group (N=288). The specimens from each material were kept under three different storage conditions (n=12): under dry conditions at room temperature; 37°C distilled water for 7 days; and 37°C distilled water for 7 days followed by 10,000 thermal cycles. All specimens were subjected to a 3-point flexural test with a crosshead speed of 1.0 mm/min. The specimens were loaded until failure. Twelve fractured specimens after the flexural test from each group were used for the Vickers hardness test (under 300 gf of loading in 15 seconds). The flexural modulus, flexural strength and Vickers hardness values were separately analyzed with two-way analysis of variance, Tukey’s multiple comparison tests at a significance level of p<0.05. There were statistically significant differences between materials and storage conditions according to flexural modulus, flexural strength and Vickers hardness values (p<0.05). The flexural strength, flexural modulus and Vickers hardness values of LU, VC, TC, VS and IC decreased after water storage followed by thermal cycling (p<0.05). The mechanical properties of provisional restoration CAD/CAM materials had showed a significantly decrease after water storage followed by thermal cycles but their mechanical properties were acceptable for fabrication of provisional restorations. The mechanical properties of VM, EC and EM were not affected by different storage conditions whereas IC and VS were affected.
scite is a Brooklyn-based organization that helps researchers better discover and understand research articles through Smart Citations–citations that display the context of the citation and describe whether the article provides supporting or contrasting evidence. scite is used by students and researchers from around the world and is funded in part by the National Science Foundation and the National Institute on Drug Abuse of the National Institutes of Health.