The microstructure of binary Al 100-x -Mg x (x = 10, 15, 18 and 25 wt%) alloys after long anneals (600-4000 h) was studied between 210 and 440°C. The transition from incomplete to complete wetting of Al/Al grain boundaries (GBs) by the second solid phase Al 3 Mg 2 has been observed. The portion of completely wetted GBs increases with increasing temperature beginning from T wsmin = 220°C. Above T wsmax = 410°C all Al/Al GBs are completely wetted by the Al 3 Mg 2 phase.
scite is a Brooklyn-based organization that helps researchers better discover and understand research articles through Smart Citations–citations that display the context of the citation and describe whether the article provides supporting or contrasting evidence. scite is used by students and researchers from around the world and is funded in part by the National Science Foundation and the National Institute on Drug Abuse of the National Institutes of Health.